Independent investment casting knowledge for global buyersB2B Network
Investment Casting Hub
Defects & Inspection

Checklist: Inspecting Castings for Shrinkage Pits

Published Updated 11 min read

Inspector examining a metal casting for surface defects under bright light
Quick answer

This checklist helps buyers identify and document shrinkage pits in investment castings during quality control. It covers visual checks, dimensional verification, and red flags for core shift, porosity, and other casting defects.

Key takeaways
  • Shrinkage pits are hollow voids that form when molten metal solidifies and pulls inward as it cools.
  • A quick visual check with a strong light source is often the fastest way to find surface pits.
  • Document every pit with its location, size, and depth so the foundry can trace the cause.
  • Compare your findings against the drawing tolerance stack before rejecting a lot of castings.

What Do Shrinkage Pits Look Like

Shrinkage pits appear as hollow voids or indentations on the casting surface. They form when the molten metal solidifies and shrinks, pulling inward as it cools. The pit may sit flush with the surface, or it may sink in a few millimeters.

Look for dark spots, craters, or rough patches. A shallow pit might look like a small hole filled with dark oxide. A deeper pit may show a distinct edge and a shadowed bottom. In aluminum castings, the bottom of a shrinkage pit often appears bright and metallic because the oxide layer is stripped away during the shrinkage event. In iron castings, the bottom is usually darker and rougher, often coated in scale.

Surface pits are the easiest to find. Internal pits are harder. They may not show until the casting is machined or tested. For this reason, a visual check is a first pass, not a final verdict. When a pit is internal, it may only reveal itself after machining exposes the void. The resulting surface will look pitted, but the void may extend deeper than the visible mark. This is why dimensional checks must always follow visual inspections.

Where to Check First

Start with the thickest sections of the part. Heat lingers there, so solidification happens later. The metal shrinks as the thinner parts have already set, creating internal stress. That stress can open a pit in the last region to freeze. A flange, a thick boss, or a large pad is the most likely place for this to happen. The surrounding thin walls solidify first and lock the structure in place. When the thick section finally freezes, it pulls the surrounding metal inward. If the metal has already set, it cannot flow to replace the lost volume. The result is a void or a pit on the surface.

Check areas where the part changes size suddenly. A large boss feeding into a thin wall is a prime spot. The heat concentrates in the boss, and the wall freezes first. The boss then shrinks and can pull the wall material into a void. Look for the pit on the thin wall, not the boss. The boss holds the heat, but the wall feels the stress. If the pit appears on the thin section, the cause is almost certainly thermal imbalance.

Also check the parting line. The two halves of the mold meet there, and any slight misalignment can trap gas. Trapped gas may condense into a pit as the metal cools. In investment casting, the parting line is often invisible after machining, but the pit remains. The pit will usually be elongated, following the path of the seam. If the pit is round, the cause is likely not the parting line.

Red Flags That Point to Core Shift

Core shift is a common cause of internal shrinkage pits. It happens when the inner core moves during pouring or as the investment cures. The core and shell move together, but the core can shift relative to the shell. That shift creates an uneven gap. Molten metal flows into the gap and freezes there, leaving a pit on the outside.

Look for pits that align with the core line. If the pit follows the path of the core, core shift is likely. Check the drawing for core lines. If the pit sits exactly where a core should be, ask the foundry for the core shift report. The report will show the movement of the core relative to the shell. If the movement exceeds the tolerance, the cause is confirmed.

A pit that is not on the core line may point to a different cause, such as poor gating or an air pocket. If the pit is isolated and away from any core line, do not assume core shift. Look at the gating system. If the gating is too small, the metal freezes before the last region fills. If the gating is too large, the metal flows too fast and traps air. Both problems can create pits, but they look different. A pit from poor gating will be in the last region to freeze. A pit from trapped air will be near the parting line or at a high point.

Quick Visual Inspection Checklist

Use this numbered list during a quick check. Print it or copy it into your inspection log.

  1. Set the casting on a clean, neutral surface. Remove any dust or wax residue.
  2. Use a strong, angled light source. Shine the light across the surface, not directly onto it.
  3. Scan the entire surface at a slow, steady pace. Move the light, not just your eyes.
  4. Mark every suspicious spot with a soft pencil. Do not erase anything yet.
  5. Measure each marked spot with calipers or a pit gauge. Record depth and width.
  6. Check the pit for a hard bottom or a loose core fragment.
  7. Photograph each pit with a scale reference.
  8. Log the findings against the drawing. Note any deviation from the tolerance.
  9. If the pit is near a machined surface, flag it for additional testing.
  10. If the pit is on a non critical surface, note it as a cosmetic issue.

This checklist is designed for speed. You can complete it in under ten minutes per part. The goal is to find the pit, not to diagnose the cause. Diagnosis comes later, with the foundry. This step is about documentation. If you miss a pit during this check, you may not find it later. The pit may be too shallow to see with the naked eye, or it may be in a shadow. The angled light source is key. It creates shadows that reveal depth. Without it, a shallow pit can look like a flat spot.

Dimensional and Tolerance Checks

A pit that sits within the tolerance may still be a defect. The drawing tolerance tells you how much material you can lose. A pit that removes material from a critical surface may violate the tolerance even if the pit is small.

Check the part against the drawing. Measure the critical dimensions. If a pit sits on a bore, a seat, or a mating surface, the dimension may be out of spec. If the pit is on a non critical surface, the dimension may still be in spec.

For example, a pit on a shaft may reduce the diameter by 0.5 mm. If the drawing tolerance is +/- 0.1 mm, the part is out of spec. The pit is a defect. A pit on a flat surface may reduce the thickness by 0.5 mm. If the drawing tolerance is +/- 0.5 mm, the part is in spec. The pit is a cosmetic issue. The difference is not the size of the pit. The difference is the location of the pit.

If the pit removes material from a critical surface, the part may need to be rejected or reworked. If the pit is on a non critical surface, it may be acceptable as a cosmetic issue. Reworking a pit on a critical surface is often not possible. You cannot add material to a pit without changing the shape. You can only remove material, which makes the pit worse. So, if the pit is on a critical surface, reject the part.

Testing Options for Internal Pits

Visual inspection finds surface pits. It does not find internal pits. For internal pits, you need non destructive testing.

X ray testing shows internal voids. It is good for checking the entire casting. It may take time and cost. Ultrasonic testing is faster and cheaper. It is good for checking specific areas. It is less effective for small pits.

For a quick check, use X ray for high value parts and ultrasonic for bulk production. For low volume, high value parts, use X ray for every part. For high volume, low value parts, use X ray for a sample and ultrasonic for the rest.

X ray testing is the gold standard for internal pits. It shows the entire internal structure. You can see the pit, the core line, and the gating. It is expensive, but it is the only way to be sure. Ultrasonic testing is a good alternative. It is faster and cheaper. It is good for checking specific areas. But it is less effective for small pits. It works by sending sound waves through the metal. If the wave hits a void, it reflects. The equipment measures the reflection. But if the void is small, the reflection is weak. The equipment may miss it.

Red Flags That Point to Other Defects

Shrinkage pits are one type of casting defect. Other defects can look similar.

Gas porosity forms small, round holes. They may cluster near the parting line. They are caused by gas in the metal. They are often smaller than shrinkage pits.

Sand inclusions are hard particles embedded in the metal. They may look like pits if they break the surface. They are caused by the investment not holding the sand.

Hot tears are cracks that form during solidification. They look like rough, irregular lines. They are caused by the metal cracking as it shrinks.

If you see a defect that does not fit the shrinkage pit profile, reclassify it. A misclassified defect can lead to the wrong corrective action.

Gas porosity is different from a shrinkage pit. Gas porosity is caused by gas trapped in the metal. The gas bubbles form as the metal solidifies. They are usually round and smooth. They may cluster near the parting line. A shrinkage pit is caused by the metal shrinking. It is usually irregular and rough. It may have a hard bottom. If you see a cluster of small, round holes, it is gas porosity. If you see a single, irregular pit, it is a shrinkage pit.

Sand inclusions are hard particles embedded in the metal. They may look like pits if they break the surface. They are caused by the investment not holding the sand. The sand particles are hard and do not shrink. They remain in the metal as the metal solidifies. If a sand particle breaks the surface, it looks like a pit. But it is not a void. It is a solid particle. You can tell by the texture. A sand inclusion is rough and hard. A shrinkage pit is smooth and hollow.

Hot tears are cracks that form during solidification. They look like rough, irregular lines. They are caused by the metal cracking as it shrinks. A hot tear is a crack, not a void. It is caused by the metal moving as it shrinks. If the metal is too thick, it shrinks too much. The crack forms where the stress is highest. A hot tear is a serious defect. It compromises the strength of the part. If you see a hot tear, reject the part.

How to Document Findings for the Foundry

A good report tells the foundry what to look for. It also protects your company if the part fails in service.

Write the date, part number, and lot number. Describe each pit with a location, size, and depth. Use a photo for each pit. Note the light source and angle.

If you suspect core shift, say so. If you suspect gas porosity, say so. If you are not sure, say so.

Attach the drawing. Mark the pit locations on the drawing. If the pit is on a critical surface, say so.

Send the report to the foundry before you accept the lot. Do not wait until the part is in service.

The report should be specific. Do not write “there is a pit.” Write “there is a pit on the top face, 10 mm from the left edge, 2 mm deep, 5 mm wide.” The foundry needs to know where the pit is to find the cause. If you do not give them the location, they cannot find the cause. If they cannot find the cause, they cannot fix it.

The report should also include the context. What is the part used for? Is it a high pressure part? Is it a low pressure part? Is it a critical part? The context helps the foundry understand the severity of the defect. A pit on a low pressure part may be acceptable. A pit on a high pressure part is not.

Red Flags That Mean the Lot Should Be Rejected

Do not accept a lot of castings if the pits are on critical surfaces. Do not accept if the pits are deep enough to affect the function. Do not accept if the pits are clustered in a pattern that points to a process failure.

A single pit on a non critical surface may be acceptable. A cluster of pits on a critical surface is not.

If the foundry cannot explain the cause, do not accept the lot. If the foundry does not provide a core shift report, do not accept the lot.

The decision to reject a lot is based on risk. If the pit is on a critical surface, the risk is high. The part may fail in service. The failure may be catastrophic. If the pit is on a non critical surface, the risk is low. The part may not fail. But if the pit is deep enough to affect the function, the risk is high.

A cluster of pits is a red flag. It points to a process failure. The foundry may have a problem with the gating, the core, or the investment. If you accept a lot with a cluster of pits, you are accepting a known problem. The problem will continue in the next lot. You are not just accepting a defect. You are accepting a process failure.

If the foundry cannot explain the cause, do not accept the lot. The cause is the most important part of the report. If they cannot find the cause, they cannot fix it. If they cannot fix it, the next lot will have the same problem. You are not just accepting a defect. You are accepting a recurring problem.

Final Thoughts

Shrinkage pits are a common casting defect. They are usually caused by the metal shrinking as it cools. A quick visual check can find most surface pits. A good report can help the foundry fix the problem.

Use the checklist above. It is simple, fast, and effective. It will help you catch the problem before it becomes a bigger problem.

Frequently asked questions

What is the difference between a shrinkage pit and gas porosity?

A shrinkage pit is a hollow void that forms when the metal shrinks as it cools. Gas porosity is a small, round hole that forms when gas is trapped in the metal. Shrinkage pits are often larger and deeper than gas porosity.

How can I tell if a pit is on a critical surface?

Check the drawing. If the pit is on a bore, a seat, or a mating surface, it is on a critical surface. If the pit is on a non critical surface, it may be acceptable as a cosmetic issue.

What should I do if I find a pit on a critical surface?

Reject the part and send it back to the foundry. Do not accept the lot. Attach a photo and a drawing mark to your report.

Can a shrinkage pit be repaired?

Some pits can be repaired by welding or filling. The repair must be approved by the foundry and your engineering team. The repair must meet the drawing tolerance.

How often should I inspect castings for shrinkage pits?

Inspect every part for high value, low volume castings. For high volume, low value castings, inspect a sample and use non destructive testing for the rest.